Welding galvanized steel sheet -
preparation, methods, zinc fumes and weld protection
Galvanized steel sheet can be welded, but not without preparation: welding galvanized steel is carried out after removing the zinc over a strip of at least 25 mm on each side of the weld, and it ends with coating repair. The arc destroys the coating in the weld and next to it, and the zinc vaporizes as zinc oxide fume. A properly prepared procedure therefore covers three elements: removing the zinc in the weld zone, extracting fumes at source and restoring corrosion protection after welding, most often with zinc-rich paint.
Data: Galvanizers Association, NIOSH, TWI, Dz.U. 2018 poz. 1286.
Why galvanized steel should not be welded without preparation
A zinc coating protects steel in two ways: it isolates it from the environment and provides sacrificial protection, corroding instead of the steel. A weld interrupts this system. The American Galvanizers Association (AGA) puts it plainly: welding destroys the zinc at the weld and damages the coating in the adjacent area. On galvanized sheet from coil the coating is also thin. According to GalvInfo Center, the Z275 designation means a minimum of 275 g/m² in total for both sides (triple-spot test average), which gives roughly 19 µm per side.
HEN-STOL calculations: 275 g/m² ÷ 2 sides ÷ 7.14 g/m² per 1 µm of zinc ≈ 19 µm per side. Conversion factor of 7.14 g/m²/µm after GalvInfo Center.
The second problem is the quality of the weld itself. TWI points out that zinc coatings generate large amounts of fume during welding, and gas trapped in the weld pool causes porosity. The risk increases in T-joints, especially with fillet welds made from both sides. The AWS D19.0 guidelines for zinc-coated steel, cited by AGA, assume that the weld is made on zinc-free steel. This is the basis of the HEN-STOL position: galvanized sheet is not welded without removing the zinc, and the coating is always restored after welding. General principles of welding the same steel without a coating are covered in the article on how bending, welding and galvanizing affect steel sheet. This text expands on the brief section there about galvanized components.
Preparing galvanized steel sheet for welding
The basis is mechanical removal of the zinc. AGA identifies grinding as the most effective method and recommends cleaning both sides of the part. Sources differ on the width of the strip: the Galvanizers Association specifies at least 25 mm on each side of the planned weld, while AGA gives a range of 1-4 inches, i.e. about 25-100 mm. In practice, a wider strip limits the amount of zinc that reaches the heat-affected zone. The Galvanizers Association adds that a slight increase in welding current helps maintain a stable arc.
Methods for welding galvanized steel sheet
Once the zinc has been removed, the weld is made on uncoated steel, in line with the assumption of AWS D19.0. This applies to arc welding, including MAG welding, widely used in production. For thin galvanized sheet, TWI describes arc braze welding (MIG brazing) with a copper-silicon CuSi3 filler wire. The filler melts below 1000 °C, the parent metal is practically not melted, and the molten filler fills the gap by capillary action. Less heat means less distortion, a narrower heat-affected zone, less zinc fume and less damage to the coating. According to TWI, the zinc around the joint still provides galvanic protection to an exposed strip about 1-2 mm wide. The method requires no flux, usually runs in short-circuit transfer, and the typical thickness range is from 0.2 mm to about 3 mm.
Comparison of approaches to joining galvanized steel sheet by welding
| Approach | Coating condition at the joint | Zinc fume | Process notes |
|---|---|---|---|
| Arc welding without removing the zinc | Destroyed in the weld and damaged next to it | High | Risk of porosity, especially in T-joints; inconsistent with the AWS D19.0 assumption of welding on zinc-free steel |
| Arc welding (e.g. MAG) after removing the zinc | Removed over a strip of min. 25 mm, to be restored | Limited | Weld on zinc-free steel in line with the AWS D19.0 assumption; coating repair required after welding |
| Arc braze welding with CuSi3 filler | Damaged in a narrow strip, approx. 1-2 mm protected galvanically | Lower | Sheet approx. 0.2-3 mm, gap approx. 0.5-1 mm, no flux, less distortion |
| Welding before hot-dip galvanizing | Continuous coating over the entire product | None (uncoated steel is welded) | Identified by the Galvanizers Association as good practice for structures |
Source: TWI, Braze welding; TWI, weld porosity; AGA, Welding Galvanized Steel; Galvanizers Association, Welding galvanized steel.
If a structure is to be welded in many places, the Galvanizers Association recommends completing all operations before hot-dip galvanizing. The coating then remains continuous, including over the welds. The differences between galvanizing finished products and the coating applied to strip at the mill are explained in the article hot-dip versus electro-galvanized coating.
Zinc fumes when welding galvanized steel and metal fume fever
At arc temperature, zinc vaporizes and oxidizes into fine zinc oxide fume. Inhaling freshly formed fume can cause temporary metal fume fever. NIOSH lists its symptoms as chills, muscle aches, nausea, fever, dry throat and cough, as well as a metallic taste and chest tightness. AGA states that symptoms appear a few hours after exposure, often at night, and full recovery usually follows within 24-48 hours. According to AGA, moderate exposure to zinc oxide has shown no lasting effects, but concentrations that cause symptoms should be avoided.
Zinc oxide exposure limits in Poland and the USA
| Indicator | Zinc oxide fume | Body |
|---|---|---|
| Recommended 8 h average limit (REL TWA) | 5 mg/m³ | NIOSH |
| Short-term limit (STEL) | 10 mg/m³ | NIOSH |
| NDS (Polish occupational exposure limit, 8 h TWA) | 5 mg/m³ | Poland, Dz.U. 2018 poz. 1286 |
| NDSCh (Polish short-term limit, 15 min) | 10 mg/m³ | Poland, Dz.U. 2018 poz. 1286 |
| Permissible average limit (PEL TWA) | 5 mg/m³ | OSHA |
Source: NIOSH Pocket Guide to Chemical Hazards: Zinc oxide. Poland: regulation of the Polish Ministry of Family, Labour and Social Policy (MRPiPS) of 12 June 2018 on maximum admissible concentrations and intensities (NDS and NDN) (Dz.U. 2018 poz. 1286), zinc oxide as Zn, inhalable fraction.
The protective measures are standard for any welding, but they matter more with galvanized steel. AGA lists dilution with fans, capture at source (hoods, at-source extraction, on-torch extraction) and air filtration. It also notes that a fixed hood may not keep concentrations below the limits, because the fume rises into the breathing zone before reaching it. The welder's position is important: a head in the fume plume significantly increases exposure. The Galvanizers Association recommends good ventilation in workshops and extraction in confined spaces, just as for uncoated steel. Where ventilation is inadequate, AGA specifies air-supplied respiratory protective equipment.
Protecting the weld after welding galvanized steel sheet
After welding, the exposed steel in the weld zone needs its protection restored. The Galvanizers Association recommends repair as soon as possible, after removing slag and other contaminants. Zinc-rich paint or paste is most commonly used, containing at least 80% zinc by weight according to the Galvanizers Association. EN ISO 1461:2022, as summarized by the Galvanizers Association, permits three renovation methods: zinc-rich paint or paste, low-melting-point zinc stick and thermal spraying of zinc to ISO 2063. The minimum repair thickness is 100 µm, unless otherwise agreed, for example where further painting is planned. The same provisions limit renovation by the galvanizer to individual areas of up to 10 cm² and a total of 0.5% of the product surface. Welds made after galvanizing fall outside this scope, which is why the extent of repair is defined in the product documentation.
Methods for restoring the coating in the weld zone
| Method | Application | Requirements and limitations |
|---|---|---|
| Zinc-rich paint or paste | Most common, applied by brush or spray | Galvanizers Association: at least 80% zinc by weight; AGA: 65-69% or over 92% zinc in the dry film |
| Low-melting-point zinc stick | Mainly horizontal surfaces | Difficult to achieve the required thickness on vertical surfaces |
| Thermal spraying of zinc (ISO 2063) | Larger surfaces | Best repair quality, but requires specialist equipment |
Source: Galvanizers Association, HDG Datasheet 4b and Datasheet 13; AGA, Zinc-Rich Paints.
AGA gives a thickness rule for zinc-rich paints: the repair coating should be 50% thicker than the surrounding zinc coating, but no thicker than 4.0 mils (about 100 µm). For Z275 sheet, with a coating of about 19 µm per side, this gives a minimum of around 29 µm, considerably less than the 100 µm cited for hot-dip galvanized products. The final value is set by the product specification. If the weld is to be painted as well, primer selection and surface preparation are covered in the article on painting galvanized steel sheet.
HEN-STOL calculations: 19 µm × 1.5 ≈ 29 µm.
Galvanized steel sheet in the HEN-STOL offer
HEN-STOL sells galvanized steel sheet without a mill certificate wholesale in thicknesses of 0.30-6.00 mm: drawing grades DX51D-DX56D, structural grades S220GD-S550GD, high-strength grades HX220LAD-HX420LAD and HCT600X-HCT980X. Zinc coatings from Z100 to Z430 are available, as well as ZM70-ZM430, ZA70-ZA255, AZ100-AZ185, ZE25-ZE75, ZF75-ZF140 and AS80-AS150, oiled or dry. For structures welded before hot-dip galvanizing, the offer also includes uncoated cold-rolled and hot-rolled steel sheet.
Sheet without a mill certificate is material sold without a mill certificate. We offer two types of material. Overrolled steel and overproduction are defect-free mill surpluses with properties like those of certified steel, cheaper solely because of the missing certificate. Second-grade sheet is material with defects that is suitable for production, and its suitability is assessed by the customer for their own process. We accept orders from 5 tonnes, with delivery throughout Europe. Coils are 100-1800 mm wide and weigh 4-24 tonnes. On request, a partner service centre cuts coils into sheets or strips, or the whole coil can be collected.
See how we can help
For parts that will be welded, the grade, coating type and coating mass, and sheet thickness all matter. Please send us the specification: steel grade, thickness, coating type and mass, oiled or dry finish, format (coil, strip or sheet) and quantity. We will check availability, advise on the choice of material for the joining process and prepare a quotation for the batch. The full range of grades, coatings and formats is presented in the HEN-STOL steel sheet offer, with separate pages for galvanized steel sheet, cold-rolled steel sheet and hot-rolled steel sheet.
Frequently asked questions
Can galvanized steel sheet be welded?
Yes, but not without preparation, because welding destroys the coating in the weld and next to it, and the zinc vaporizes as zinc oxide fume. If welding is necessary, the zinc is first removed over a strip of at least 25 mm on each side of the weld, fume extraction is provided at source, and after welding the protection is restored with zinc-rich paint or paste.
How wide a strip of zinc is removed before welding?
The Galvanizers Association specifies at least 25 mm on each side of the planned weld, and the American Galvanizers Association a range of 1-4 inches, i.e. about 25-100 mm. The coating is removed from both sides of the sheet, most effectively by grinding. A wider strip limits the amount of zinc in the heat-affected zone and the risk of weld porosity.
What is metal fume fever when welding galvanized steel?
It is a temporary illness caused by inhaling fresh zinc oxide fume. The symptoms resemble flu: chills, muscle aches, fever, dry throat, cough and a metallic taste. They appear a few hours after exposure and, according to AGA, usually subside within 24-48 hours. It is prevented by fume extraction at source and adequate ventilation.
Is MIG brazing suitable for galvanized steel sheet?
According to TWI, yes, especially for thin sheet from about 0.2 to 3 mm. CuSi3 filler melts below 1000 °C, so there is less zinc fume, less distortion and a narrower heat-affected zone. The zinc at the joint still provides galvanic protection to an exposed strip about 1-2 mm wide. The method requires no flux.
How should a weld on galvanized steel sheet be protected?
After removing the slag, zinc-rich paint or paste containing at least 80% zinc by weight is applied. The Galvanizers Association summary of EN ISO 1461 gives a minimum repair thickness of 100 µm, unless otherwise agreed. Alternatives are zinc sticks and thermal spraying of zinc to ISO 2063.
Which is better: welding galvanized steel or galvanizing after welding?
For structures with many welds, the Galvanizers Association identifies completing all operations before hot-dip galvanizing as good practice. The coating is then continuous over the entire product, including the welds. If sheet that is already galvanized has to be welded, this usually involves individual joints and requires removing the zinc and repairing the coating.
Sources
- American Galvanizers Association, Welding Galvanized Steel and Zinc-Rich Paints (Knowledgebase)
- Galvanizers Association, Welding galvanized steel; HDG Datasheet 4b: Hot Dip Galvanizing to EN ISO 1461:2022, 2024; HDG Datasheet 13: Coating Repair, 2023
- TWI, Braze welding (Job Knowledge 134) and Defects/imperfections in welds: porosity
- NIOSH, Pocket Guide to Chemical Hazards: Zinc oxide; Regulation of the Polish Minister of Family, Labour and Social Policy of 12 June 2018 on maximum admissible concentrations and intensities of agents harmful to health in the working environment (Dz.U. 2018 item 1286, as amended), Annex 1: zinc oxide
- International Zinc Association (GalvInfo Center), GalvInfoNote 1.1: Understanding Coating Weight Designations for Zinc-Based Coatings on Steel Sheet, 2020