Galvanic (bimetallic) corrosion is the accelerated corrosion of a less noble metal in contact with a more noble one in the presence of an electrolyte; according to GalvInfo, zinc in contact with copper corrodes at 3.2 µm/year in a marine atmosphere, compared with 1.3 µm/year with no contact with another metal. On galvanized steel, the zinc is the anode and it is the zinc that corrodes. The extent of the effect depends on the metal pair, the environment and the area ratio. Copper is a clearly unfavourable pairing, stainless steel is usually not a serious problem in the atmosphere, and aluminium is practically compatible with zinc in the atmosphere.
Data: American Galvanizers Association, GalvInfo Center (International Zinc Association). HEN-STOL calculations: 1.10 V - 0.86 V = 0.24 V.
How galvanic corrosion occurs
Two dissimilar metals in contact and bridged by an electrolyte form a cell. The Galvanizers Association likens this to a battery in which current flows, and the more electronegative metal, the anode, corrodes faster. The American Galvanizers Association (AGA) lists four necessary conditions: an anode that gives up electrons, a cathode that accepts them, an electrolyte that conducts ions and a return current path, usually direct metal-to-metal contact. Remove any one of them and the process stops. The GalvInfo Center stresses that galvanic corrosion attacks only one of the two metals, and that the electrolyte can be condensation, dew, rain, damp deposits or soil moisture.
This is precisely the mechanism that makes zinc work on steel: it is anodic to steel and protects it at scratches and cut edges. The AGA, however, points out the other side of the coin. If zinc becomes the anode in a pair with a metal more noble than steel, it is consumed protecting that joint rather than the steel underneath. We cover how different coatings protect steel in more detail in our article on types of steel sheet coatings.
Galvanic series
The direction of the reaction is determined by the position of the metals in the galvanic series. The greater the potential difference, the greater the tendency to corrode. The SCI cautions, however, that the potential difference alone is a poor predictor of actual risk, because oxide films, the area ratio and the composition of the electrolyte also matter.
For guidance, the AGA gives the following potentials in seawater: zinc -1.10 V, aluminium -0.86 V, carbon steel -0.68 V. Copper and stainless steel are both more noble than zinc, so in each of the pairs described below the zinc remains the anode.
Metals in contact with galvanized steel: risk of additional zinc corrosion
| Metal in contact | Rural atmosphere | Urban and industrial atmosphere | Marine atmosphere | Seawater |
|---|---|---|---|---|
| Aluminium | 0 | 0-1 | 0-1 | 1-2 |
| Stainless steel | 0-1 | 0-1 | 0-1 | 1-2 |
| Copper | 0-1 | 1-2 | 1-2 | 2-3 |
Source: Galvanizers Association, HDG Datasheet 10: Bimetallic Corrosion, 2024. Scale: 0 none or very slight additional corrosion, 1 slight to moderate, 2 fairly severe, protection usually required, 3 severe, contact should be avoided.
Factors that govern galvanic corrosion
Electrolyte and environment
According to the Galvanizers Association, the risk in dry interiors is very low, it increases outdoors with rain and condensation, and the worst case is immersion, where the electrolyte permanently connects the metals. The AGA adds that rainwater and dew are weak electrolytes because they contain little salt. Marine atmospheres and meltwater containing road salt are strong electrolytes. The SCI highlights time of wetness: good ventilation and free drainage limit the attack, while damp crevices and standing water accelerate it.
Anode-to-cathode area ratio
This is often the decisive factor. The corrosion current is distributed over the anode surface, so a small anode in a large cathode corrodes quickly and deeply. The AGA illustrates this with two examples. A zinc rivet in a stainless steel plate will fail quickly. A stainless steel rivet in a zinc plate spreads the attack over a large area and, according to the AGA, should not fail by corrosion, because the penetration is shallow. The Galvanizers Association adds that with a rating of 0 or 0-1 and a large zinc area, no significant additional corrosion is expected.
Zinc corrosion rates in galvanic couples (µm/year)
| Zinc in contact with | Rural atmosphere | Urban atmosphere | Marine atmosphere |
|---|---|---|---|
| Zinc with no contact (reference) | 0.5 | 2.4 | 1.3 |
| Aluminium | 0.4 | 1.1 | 1.1 |
| Stainless steel | 1.1 | 1.8 | 2.0 |
| Copper | 2.2 | 2.0 | 3.2 |
| Carbon steel | 3.0 | 3.3 | 3.9 |
Source: GalvInfo Center (International Zinc Association), GalvInfoNote 3.6, results of exposure tests on galvanic couples.
The GalvInfo table shows that in a rural atmosphere contact with carbon steel increases zinc corrosion 6-fold and contact with copper 4.4-fold, while in a marine atmosphere the figures are 3-fold and 2.5-fold respectively (HEN-STOL calculations: rate in the couple / rate of zinc with no contact). In its description, GalvInfo gives rounded values: up to 5 times in a rural atmosphere and up to 3 times in a marine one. Ordinary carbon steel proved to be the strongest cathode, partly because its rust retains moisture and contaminants. This matters for exposed edges and scratches on galvanized steel sheet, where the zinc works for the steel exactly as intended.
Typical cases: stainless steel, copper, aluminium
Stainless steel screws and fasteners in galvanized steel sheet
This is the most common pairing in practice. A small stainless fastener is a cathode with a small area, and the galvanized sheet is an anode with a large area, so the arrangement is favourable. The SCI rates contact between galvanized and stainless steel as usually harmless, except in aggressive marine environments. The Galvanizers Association gives this pair a rating of 0-1 in the atmosphere, yet still recommends insulating washers as good practice. Under immersion the effect is markedly stronger: in seawater the rating is 1-2 and separating the metals is recommended. The reverse configuration, a galvanized fastener in a large stainless steel component, is unfavourable, because the small anode is quickly consumed.
Copper and run-off water from copper
Copper is the pairing best avoided. The Galvanizers Association recommends electrical insulation even in the atmosphere and a design that prevents water from copper running onto galvanized surfaces. GalvInfo describes a mechanism that works without any metal-to-metal contact: copper dissolved in water deposits on the zinc and displaces it. In the case described, an air-conditioning unit frame, corrosion was severe where the copper pipes passed through and less severe where copper-bearing condensate dripped. The AGA recommends that water should flow from the galvanized surface towards the copper, not the other way round, and that it should not be recirculated.
Aluminium in contact with galvanized steel
The potential difference is small, about 0.24 V in seawater, and aluminium forms an insulating surface film. The AGA considers a reaction unlikely, and GalvInfo regards zinc and aluminium as galvanically compatible in the atmosphere. In measurements, zinc corrosion in a couple with aluminium was even lower than with no contact. The Galvanizers Association nevertheless recommends insulation for large aluminium claddings and rates the risk in seawater at 1-2. White deposits on galvanized surfaces at such locations are not necessarily caused by the galvanic couple. More often they are white rust on galvanized steel sheet, linked to moisture and poor ventilation.
How to prevent galvanic corrosion
The durability of the coating itself also depends on its type and mass. A thicker zinc coating has a larger reserve of material, and zinc-magnesium coatings with different corrosion behaviour are described in our article on Magnelis steel sheet. No coating, however, replaces insulating a joint with copper.
Galvanized steel sheet in the HEN-STOL offer
HEN-STOL sells galvanized steel sheet without a mill certificate wholesale in thicknesses of 0.30-6.00 mm: deep-drawing grades DX51D-DX56D, structural grades S220GD-S550GD, high-strength grades HX220LAD-HX420LAD and HCT600X-HCT980X. Available coatings include zinc from Z100 to Z430, zinc-magnesium ZM70-ZM430, as well as ZA70-ZA255, AZ100-AZ185, ZE25-ZE75, ZF75-ZF140 and AS80-AS150, oiled or dry.
Sheet without a mill certificate is material sold without a certificate issued by the steel mill. Overrolled steel and overproduction are defect-free mill surpluses with properties like those of certified steel, cheaper solely because of the missing certificate. Second-grade sheet is material with defects that is still suitable for production, and the customer assesses its suitability for their own process. We accept orders from 5 tonnes, with delivery throughout Europe. Coils are 100-1800 mm wide and weigh 4-24 t; on request, a partner service centre cuts coils into sheets or strips.
See how we can help
Choosing the coating for the specific service environment and joining method affects the durability of the entire structure. Please send us the specification: steel grade, thickness, coating type and mass, oiled or dry finish, format (coil, strip or sheet) and quantity. We will check availability, advise on the choice of coating and prepare a quotation for the batch. The full range of grades, coatings and formats is presented in the HEN-STOL steel sheet offer, with separate pages for galvanized steel sheet, cold-rolled steel sheet and hot-rolled steel sheet.
Frequently asked questions
What is galvanic corrosion?
It is the accelerated corrosion of a less noble metal in contact with a more noble metal in the presence of an electrolyte, such as water or condensation. A cell is formed in which the anode corrodes faster. Four elements are required: an anode, a cathode, an electrolyte and an electrical connection. Removing any one of them stops the process.
Can galvanized steel sheet be fixed with stainless steel screws?
In the atmosphere, usually yes. A small stainless fastener in a large galvanized area gives a favourable area ratio, and the Galvanizers Association rates this pair at 0-1, meaning no or slight additional corrosion. As good practice, however, it recommends insulating washers. Under immersion, especially in seawater, separating the metals is recommended.
Why is copper harmful to galvanized steel?
Copper is much more noble than zinc, so zinc in contact with it corrodes faster. GalvInfo reports up to 3.2 µm/year in a marine atmosphere. Run-off water from copper is also harmful: dissolved copper deposits on the zinc and displaces it, even without direct metal-to-metal contact. Insulation and the correct run-off direction are recommended.
Can aluminium and galvanized steel be in contact?
In the atmosphere, yes. The potential difference is about 0.24 V, and aluminium is protected by an insulating surface film. GalvInfo regards these metals as galvanically compatible in the atmosphere, and in tests zinc corrosion in a couple with aluminium was lower than with no contact. For large claddings and in seawater, insulation is recommended.
How does the area ratio affect galvanic corrosion?
It is decisive. The corrosion current is distributed over the anode surface, so a small anode in a large cathode corrodes quickly and deeply. According to the AGA, a zinc rivet in a stainless steel plate will fail quickly, whereas a stainless steel rivet in a zinc plate should not fail, because the attack is spread over a large area.
How can galvanic corrosion of galvanized steel be prevented?
The most effective measure is to break the electrical connection: neoprene or plastic washers, insulating spacers and gaskets. Choosing fasteners of the same or a similar metal helps, as does painting the joint or, where that is not possible, painting the more noble metal. Free drainage and avoiding run-off from copper onto galvanized surfaces are also important.
Sources
- American Galvanizers Association, Stainless Steel in Contact with Galvanized Steel; Galvanized Steel with Aluminum Parts; In Contact with Other Metals
- Galvanizers Association, HDG Datasheet 10: Bimetallic Corrosion, 2024
- International Zinc Association (GalvInfo Center), GalvInfoNote 3.6: Galvanic/Bimetallic (including Cut Edge) Corrosion of Galvanized Sheet, 2017
- Steel Construction Institute, New Steel Construction AD 339: Stainless steel in contact with other metals, 2009
- SteelConstruction.info (BCSA, SCI, Tata Steel), Corrosion of structural steel