DD11 steel sheet -
hot-rolled steel for cold forming to EN 10111, properties and applications
DD11 steel sheet is a hot-rolled low-carbon steel for cold forming to EN 10111, with a carbon content of up to 0.12%, a yield strength of 170-340 MPa (for thicknesses of 2-11 mm) and a tensile strength of no more than 440 MPa. DD11 is the first grade in the DD11-DD14 series: each subsequent grade has lower limits for manganese, phosphorus and sulphur, a lower upper limit of tensile strength and higher elongation, so it performs better in drawing operations. DD11 is chosen for bending, simple stamping, sections and tubes, in other words wherever predictable behaviour of the sheet in the press matters more than minimum load-bearing capacity.
Data: EN 10111:2008 as per the Salzgitter Flachstahl and ArcelorMittal data sheets, scope of the standard as per EVS (CEN).
What DD11 steel is and what EN 10111 covers
EN 10111:2008 is the European standard for continuously hot-rolled flat products made of low-carbon steels intended for cold forming. It applies to sheet and strip supplied in coils with thicknesses from 1 to 11 mm, covering both wide strip (from 600 mm) and slit strip. For each grade, the standard specifies the chemical composition and mechanical properties. It does not cover structural steels to EN 10025 or steels for pressure vessels and gas cylinders, which have their own standards.
In older German documentation, according to thyssenkrupp Steel, DD11 appears as StW22, DD12 as RRStW23 and DD13 as StW24.
Mills also produce these grades in thicknesses above 11 mm (thyssenkrupp and ArcelorMittal up to 16 mm), but the mechanical properties are then agreed individually, as they fall outside the scope of the standard.
Chemical composition of DD11, DD12, DD13 and DD14
The differences between the grades start with the chemistry. The lower the carbon, manganese, phosphorus and sulphur content, the softer and more ductile the steel. According to the Salzgitter Flachstahl data sheet, unless otherwise agreed in the order, nitrogen-binding elements such as titanium and boron may be added to these grades.
Chemical composition of DD11-DD14 steels to EN 10111 (cast analysis, % by mass, max.)
| Grade | C | Mn | P | S |
|---|---|---|---|---|
| DD11 | 0.12 | 0.60 | 0.045 | 0.045 |
| DD12 | 0.10 | 0.45 | 0.035 | 0.035 |
| DD13 | 0.08 | 0.40 | 0.030 | 0.030 |
| DD14 | 0.08 | 0.35 | 0.025 | 0.025 |
Source: Salzgitter Flachstahl, Steel grades - mild non-alloy steels for direct cold-forming; ArcelorMittal, catalogue A10.
Mills often tighten these limits in their own variants. In DD11 AM FCE, ArcelorMittal limits sulphur to 0.030% and adds a requirement of min. 0.010% aluminium, while thyssenkrupp specifies max. 0.015% sulphur for DD13 precision strip. These are, however, manufacturer specifications, not requirements of the standard.
Mechanical properties of DD11 compared with DD12-DD14
For EN 10111 grades, mill data sheets give the yield strength not as a single minimum value but as a range. The lower limit of 170 MPa is common to all grades, and the difference lies in the upper limit: the lower it is, the more consistent the forming. Salzgitter Flachstahl states that tensile test specimens are taken transverse to the rolling direction, provided the product width allows it.
Mechanical properties of DD11-DD14 steels to EN 10111
| Grade | Re [MPa], thickness < 2 mm | Re [MPa], thickness 2-11 mm | Rm max. [MPa] | A min. [%] < 2 / 2-3 / 3-11 mm |
|---|---|---|---|---|
| DD11 | 170-360 | 170-340 | 440 | 23 / 24 / 28 |
| DD12 | 170-340 | 170-320 | 420 | 25 / 26 / 30 |
| DD13 | 170-330 | 170-310 | 400 | 28 / 29 / 33 |
| DD14 | 170-310 | 170-290 | 380 | 31 / 32 / 36 |
Source: Salzgitter Flachstahl; ArcelorMittal, catalogue A10; Nippon Steel Slovakia, Drawing steel. The gauge length of the test piece used to determine elongation depends on the thickness range; mill data sheets state it in the table headers.
The table gives a practical selection rule. DD11 has the widest yield strength range and the lowest elongation, so it works well for bending and shallow drawing. At thicknesses of 3-11 mm, DD14 provides at least 36% elongation with Rm up to 380 MPa, which leaves a margin for deep drawing. Nippon Steel Slovakia puts it plainly: DD11 for less demanding pressings and bending, DD12 for moderately difficult drawing, DD13 for drawing and surface-treated parts, DD14 for the most difficult pressings.
Tata Steel specifies a mandrel diameter of 1t (equal to the sheet thickness) in the bend test for DD11. This is an acceptance test value, not a recommended bending radius for production.
DD11 vs S235JR: which steel to use when
Both steels are hot-rolled and often sit side by side in the same warehouse, but they serve different purposes. For S235JR to EN 10025-2, mill data sheets give minimum values: a yield strength of at least 235 MPa for thicknesses up to 16 mm, Rm of 360-510 MPa and an impact energy of 27 J at 20°C. These are parameters for the structural designer calculating load-bearing capacity. For DD11, by contrast, mill data sheets give upper limits: Re max. 340-360 MPa and Rm max. 440 MPa. What matters to a press shop engineer is precisely that the sheet will not turn out too hard for the tool.
DD11 vs S235JR (selected parameters)
| Parameter | DD11 (EN 10111) | S235JR (EN 10025-2) |
|---|---|---|
| Intended use | cold forming: bending, drawing | steel structures, load-bearing members |
| Yield strength | 170-340 MPa (2-11 mm) | min. 235 MPa (up to 16 mm) |
| Tensile strength | max. 440 MPa | 360-510 MPa |
| Impact energy | no requirements given in mill data sheets | 27 J at 20°C |
| Thickness tolerance, up to 2 mm, width up to 1200 mm | ±0.13 mm | ±0.17 mm (category A) |
Source: Salzgitter Flachstahl; Arvedi, Non-alloyed structural steels as per EN 10025-2; Nippon Steel Slovakia, Structural steel (EN 10051 tolerances, category A, for Re ≤ 300 MPa); Tata Steel, Steel for forming (DD11-DD14 tolerances to EN 10051).
The detailed properties of structural steels are covered in the article on S235JR and S355JR steel. When good formability and higher strength are needed at the same time, the next step is the microalloyed steels of EN 10149-2, described in the article on S355MC-S700MC steel.
Applications of DD11 steel sheet
Mills list a similar set of applications for DD11-DD14 steels. They have one thing in common: the part is made by bending, drawing or blanking, and its shape matters more than high load-bearing capacity.
DD grades can be welded by all common methods without preheating, as Salzgitter Flachstahl states in its product data sheet. This makes it easier to produce welded structures from bent parts.
Pickled and unpickled surface
Hot-rolled sheet leaves the rolling mill covered with mill scale, a layer of oxides. Pickling removes this layer by chemical and mechanical means, and oiling protects the cleaned surface against corrosion during storage. Tata Steel gives a typical oil coating weight of 0.5-2.5 g/m². According to voestalpine, unpickled material is supplied unoiled only.
The choice depends on further processing. Pickled sheet has a clean, oxide-free surface, and thyssenkrupp stresses that the high surface quality of DD grades favours finishing and coating. Unpickled sheet retains its mill scale. Tata Steel also points out that trimmed edges are available only for pickled material. The differences between hot-rolled and cold-rolled products are described in the article hot-rolled vs cold-rolled steel sheet.
DD11 steel sheet in the HEN-STOL offer
HEN-STOL wholesales hot-rolled steel sheet in thicknesses of 1.20-100 mm, including the cold-forming grades DD11, DD12, DD13 and DD14. The material is available pickled and oiled or unpickled (dry), in coils 100-1800 mm wide and weighing 4-24 t. On request, a partner service centre cuts coils into sheets or strips.
We offer steel without a mill certificate, that is, material sold without the mill's certification, in two variants. Overrolled steel and overproduction are defect-free mill surpluses with properties like those of certified steel, cheaper solely because there is no mill certificate. Second-grade sheet has defects but is suitable for production, and the customer assesses its suitability for their own process. We accept orders from 5 tonnes, with delivery throughout Europe.
See how we can help
For bending and simple stamping, DD11 is usually sufficient, while DD13 or DD14 perform better in deeper pressings. Please send us the specification: grade, thickness, width, surface type (pickled or unpickled), delivery form (coil, strip, sheet) and quantity. We will check availability, advise on the choice of grade and prepare a quotation. The full range of grades, coatings and formats is presented in the HEN-STOL steel sheet offer, with separate pages for galvanized steel sheet, cold-rolled steel sheet and hot-rolled steel sheet.
Frequently asked questions
What is DD11 steel?
DD11 is a hot-rolled low-carbon steel for cold forming to EN 10111. It contains up to 0.12% carbon and up to 0.60% manganese, and has a yield strength of 170-340 MPa at thicknesses of 2-11 mm and a tensile strength of no more than 440 MPa. It is used for bending, simple stamping and the production of tubes, sections and machine components.
How does DD11 differ from DD13 and DD14?
Each subsequent grade has lower limits for manganese, phosphorus and sulphur (and for carbon from DD11 to DD13), lower upper limits of yield and tensile strength, and higher elongation. At thicknesses of 3-11 mm, DD11 has min. 28% elongation and DD14 min. 36%, with Rm up to 380 MPa. DD11 is used for bending and shallow drawing, DD13 for drawing and DD14 for the most difficult pressings.
Can DD11 be used instead of S235JR?
Only in parts that are not designed as load-bearing. The lower yield strength limit of DD11 is 170 MPa and mill data sheets give no impact requirements for this grade, whereas S235JR has min. 235 MPa and 27 J at 20°C. On the other hand, DD11 has a capped upper strength, which makes bending and drawing easier. The choice depends on whether load-bearing capacity or formability is the deciding factor.
What thickness range does EN 10111 cover?
EN 10111:2008 covers hot-rolled flat products in coils with thicknesses from 1 to 11 mm. Mills also produce DD grades in greater thicknesses, for example up to 16 mm, but the mechanical properties are then agreed individually with the manufacturer, as they fall outside the scope of the standard.
When should you choose pickled DD11 sheet and when unpickled?
Pickling removes mill scale, and oil protects the surface against corrosion during storage. Pickled sheet is chosen for painted and coated products and wherever a clean surface matters. Unpickled sheet retains its mill scale and, according to voestalpine, is supplied without oil. Both variants are available from HEN-STOL.
Is DD11 steel weldable?
Yes. Salzgitter Flachstahl states in its product data sheet that DD11-DD14 grades can be welded by all common methods without preheating. ArcelorMittal adds that the spot and arc weldability of hot-rolled DD grades is the same as that of the corresponding cold-rolled grades. For DD14 AM FCE with a thickness of 2.5 mm, the mill gives a spot welding current range of 9.6-12.6 kA.
Sources
- Estonian Centre for Standardisation and Accreditation (EVS), EN 10111:2008 Continuously hot rolled low carbon steel sheet and strip for cold forming - Technical delivery conditions, description of the standard, 2008
- Salzgitter Flachstahl, Steel grades - mild non-alloy steels for direct cold-forming, grade data sheet DD11-DD14
- ArcelorMittal, Hot rolled steels for cold forming and deep drawing, catalogue A10
- Tata Steel, Hot rolled steel for forming DD11, product data sheet
- Nippon Steel Slovakia, Drawing steel and Structural steel, grade data sheets DD11-DD14 and S235JR